Technical Data Sheet
Alloy 825 is a nickel-iron-chromium alloy with additions of molybdenum and copper. It has excellent resistance to both reducing and oxidizing acids, to stress-corrosion cracking, and to localized attack such as pitting and crevice corrosion. Alloy 825 is especially resistant to sulfuric and phosphoric acid. Alloy 825 is used for chemical processing, pollution control equipment, oil and gas well piping, nuclear fuel reprocessing, acid production and pickling equipment and handling of radioactive wastes.
| Chemical Composition Limits | |||||||||||
| Weight % | Ni | Fe | Cr | Mo | Cu | Ti | C | Mn | S | Si | Al |
| Alloy 825 | 38 – 46 | 22 min | 19.5 – 23.5 | 2.5 – 3.5 | 1.5 – 3 | 0.6 – 1.2 | 0.05 max | 1 max | 0.03 max | 0.5 max | 0.2 max |
Typical Mechanical Properties
| Material | Form and Condition | Tensile Strength MPa | Yield Strength (0.2% Offset) MPa | Elongation (%) |
| Alloy 825 Tube | Annealed | 772 | 441 | 36 |
| Alloy 825 Tube | Cold Drawn | 1000 | 889 | 15 |
| Alloy 825 Bar | Annealed | 690 | 324 | 45 |
| Alloy 825 Plate | Annealed | 662 | 338 | 45 |
| Alloy 825 Sheet | Annealed | 758 | 421 | 39 |