Technical Data Sheet
Nickel Alloy 600 (N06600) is a nickel-chromium-iron alloy with good oxidation resistance at high temperatures and resistance to chloride-ion stress corrosion cracking corrosion by high-purity water, and caustic corrosion. Alloy 600 also has excellent mechanical properties and has a desirable combination of high strength and good workability. Used for furnace components, in chemical and food processing, in nuclear engineering and for the sparking electrodes.
| Chemical Composition Limits | ||||||||
| Weight% | C | S | Cr | Cu | Mn | Si | Ni | Fe |
| Nickel Alloy 600 | 0.15 max | 0.015 max | 14.0 – 17.0 | 0.50 max | 1.0 max | 0.50 max | 72.0 min | 6 – 10 |
Typical Mechanical Properties
| Material | Form and Condition | Tensile Strength | Yield Strength | Elongation % | Hardness, Rockwell | ||
| ksi | MPa | ksi | MPa | ||||
| Alloy 600 rod and bar | Cold drawn Annealed | 80-100 | 550-690 | 25-50 | 170-345 | 55-35 | 65-85B |
| Alloy 600 Plate | Hot rolled Annealed | 80-100 | 550-725 | 30-50 | 205-345 | 55-35 | 65-85B |
| Alloy 600 Sheet | Cold Rolled Annealed | 80-100 | 550-690 | 30-45 | 205-310 | 55-35 | 88B max |
| Alloy 600 Tube and Pipe | Cold Drawn Annealed | 80-100 | 550-690 | 25-50 | 170-345 | 55-35 | 88B max |
| Alloy 600 Wire | Cold Drawn Annealed | 80-120 | 550-830 | 35-75 | 240-520 | 45-20 | – |
| Alloy 600 Wire | Cold Drawn No. 1 Temper | 105-135 | 725-930 | 70-105 | 480-725 | 35-15 | – |
| Alloy 600 Wire | Spring Temper | 170-220 | 1170-1520 | 150-210 | 1035-1450 | 5-2 | – |